Is your filament wet? Wet filament tends to be brittle.
Post pics of your first layer and final print.
3DPrinting is a place where makers of all skill levels and walks of life can learn about and discuss 3D printing and development of 3D printed parts and devices.
The r/functionalprint community is now located at: !functionalprint@kbin.social or !functionalprint@fedia.io
There are CAD communities available at: !cad@lemmy.world or !freecad@lemmy.ml
No bigotry - including racism, sexism, ableism, homophobia, transphobia, or xenophobia. Code of Conduct.
Be respectful, especially when disagreeing. Everyone should feel welcome here.
No porn (NSFW prints are acceptable but must be marked NSFW)
No Ads / Spamming / Guerrilla Marketing
Do not create links to reddit
If you see an issue please flag it
No guns
No injury gore posts
If you need an easy way to host pictures, https://catbox.moe/ may be an option. Be ethical about what you post and donate if you are able or use this a lot. It is just an individual hosting content, not a company. The image embedding syntax for Lemmy is ![](URL)
Moderation policy: Light, mostly invisible
Is your filament wet? Wet filament tends to be brittle.
Post pics of your first layer and final print.
it could be a few things... to start off with, what's the ambient temperature inside the enclosure? how cold is 'cold'?
Regardless, first step is probably to print a temperature calibration tower. (Most PLA I've used prints much more happily at 215-225,) I like this version of it. there's ways to set up the slicer to change the temperature at a given height. (For prusa, in the sliced preview pain, you can right click, it's the same menu as 'color change' and stuff. Start high and work low, going about five or ten degrees at a time.)
If the tower comes out no different and still brittle/poor adhesion across the full range... then my first thought is thermal stress building up in the part. if your enclosure is still too gold, consider piling on some more insulation (a generic quilt or blanket over, or stapled around inside will do nicely. Cotton quilts also have the advantage of being difficult to set on fire/melt.)
you say the part is brittle- does it snap opposite layer lines? or along layers? if it breaks in directions not aligned with the layer lines as easily as it does aligned, then it's probably not layer issues... at that point you have some sort of material issue. I'd suggest drying your filament out, and doing what you can to minimize the temperature changes during printing.
How cold is cold?
The printer says the hot end and bed are both ambient at 10C , which is 50F. For reference, it's 21F outside right now.
Also, here is a picture of where it broke. The other print was similar. The crack can be seen on the left side of the pic.
Also, I think my nozzle is clogged now, all of a sudden my first layers have gone to garbage. Compounding failures lol
the printer says the hot end and bed are both ambient at 10C
Try leaving the hot end at ambient, turning on the heat bed to it's printing temperature. Give it a while for everything to come up inside. considering room temp is around 20-22c or 68-73 F, it's not quite as bad as i feared, but it could be better.
The heat bed should be able to warm it up a bit, but that is a very sharp differential, and drafts will cause problems. One thing to maybe try, is printing a tall brim. (basically a single-wall perimeter close to the part. They're not as useful if you have an enclosure, but they can help shield a draft and keep some of the heat in from the bed better.)
Clogging could have happened if you're trying to print too low in temperature, which, given the layer problems, that also looks likely. there's a few variations, but you can try a cold pull to clear the nozzle (especially if it's only partially clogged.)
My apologies, that room temperature is around 25° f, which is -4c. It's very cold.
I just performed a cold pull, seemed to go okay, it was my first one. I feel like the majority of my problems here is simply trying to print when it's so damn cold outside lol
Edit: The cold pull definitely seemed to completely solve my first layer issues, great suggestion. I threw a blanket over the next print, we'll see if that helps
My apologies, that room temperature is around 25° f, which is -4c. It’s very cold
yeah. so, what's your enclosure like? is it fully enclosed? one of those tent-thingies?
I'd suggest considering some type of insulation. Blankets work- if it's MDF or mealmine or plywood, stappling them inside. If... insulation is problem... Blankets over a big-enough cardboard box work (just be aware of melting/fire risks. Cotton>synthetics. card board is okay. my old I3 prusa had cardboard under the heat bed instead of cork or neoprene for a long time. Try to keep it small enough to just fit everything inside. (cut the top flaps off and put it over upside down.)
The heat bed should be good enough to get it most the way there- and if you find it takes too long to heat up the inside... a heat gun can prime things nicely.
Yep, it's the official creality enclosure. I threw a quilt over it, so here goes
-4c is extreemly cold, get thermometer inside of enclosure and leave your heatbed on until it reaches 10-15C before you start printing. Even better get enclosure heater. Id also bump nozzle temp to the highest marked on your spool.
Crossing my fingers for yah.
Ok, so the print came out great. Unfortunately, it was a print without top and bottom layers and honeycomb infill of only about 12%, and I accidentally squished it getting it off that extremely cold bed this morning lol. To the immediate problem I posted above though, I think it was definitely a clogged nozzle which you helped fix, and the layer adhesion is probably due to enclosure temperature being too low when I start the print. I will correct both of those things, and then go watch YouTube on how to remove a print from a cold bed haha
So, one of the tricks for really stuck on prints, at least for glass beds, is to put it in the freezer and then hold the build plate vertically and tap it on something hard. (Firm, but not so hard it breaks or anything.) my experience in the past is, with some exceptions... it goes in the freezer and pops right off. if bed adhesion is too good, you can try adjusting zoffset to print a little higher.
you can speed warming up the enclosure with a hairdryer or heat gun.
What have your first layers looked like before this? The hard to remove skirt on prior prints is usually from your nozel being too close to your bed.
Before this they were typically ok - I did tram the bed again using a sticky note just to be safe. However, since I'm new, i'm still getting a feel (literally) for how much resistance is correct. Would a print sticking too much to the bed be an indication my z offset is too low (meaning nozzle too close) ? Typically people complain about too little adhesion, and i have too much lol
Yes, leveling too low can give you very strong adhesion. It's worth noting that PEI beds tend to lose adhesion as they and the print cool down. I can remove cooled prints without much effort off my bed, bit hot prints take some more convincing.
You can set nozzle distance with a mechanical feeler, like your sticky note, but you will need to fine tune some based on things like extrusion temperature and type of filament. This guide was made for printers with auto bed leveling, but the pictures are helpful.
Here are some signs you're too close to the bed:
That sounds exactly like my problem, I will adjust, thank you very much
You might consider the ambient temperature in your printer space
New Lemmy Post: Issues with layer adhesion (i think) (https://lemmy.world/post/9732230)
Tagging: #3dprinting
(Replying in the OP of this thread (NOT THIS BOT!) will appear as a comment in the lemmy discussion.)
I am a FOSS bot. Check my README: https://github.com/db0/lemmy-tagginator/blob/main/README.md